Raddied | 0cr27al7mo2 |
Maint | 0.1-1.2mm |
Wyneb | Annealed Disglair |
Mhwysedd | 1-3kg/rholio |
Gwrthsefyll | 1.53 ± 0.07μΩ.m |
Y tymheredd uchaf | 1400 ℃ |
Ddwysedd | 7.1g/cm³ |
Cryfder tynnol | 750n/mm² |
Hehangu | ≥10% |
Paramentwyr Cynnyrch
Raddied | Y tymheredd uchaf | Gwrthsefyll | Pwynt toddi | Cryfder tynnol | Hehangu |
0cr21al4 | 1100 ℃ | 1.23 ± 0.06μω.m | 1500 ℃ | 750 | ≥12 |
0cr25al5 | 1250 ℃ | 1.42 ± 0.07μω.m | 1500 ℃ | 750 | ≥12 |
0cr23al5 | 1300 ℃ | 1.35 ± 0.06μΩ.m | 1500 ℃ | 750 | ≥12 |
0cr21al6nbco | 1350 ℃ | 1.43 ± 0.07μω.m | 1510 ℃ | 750 | ≥12 |
0cr27al7mo2 | 1400 ℃ | 1.53 ± 0.07μΩ.m | 1520 ℃ | 750 | ≥10 |
Csc | 1350 ℃ | 1.44 ± 0.05μω.m | 1510 ℃ | 750 | ≥16 |
Cr20ni80 | 1200 ℃ | 1.09 ± 0.05μΩ.m | 1400 ℃ | 750 | ≥20 |
Cr15ni60 | 1150 ℃ | 1.12 ± 0.05μΩ.m | 1390 ℃ | 750 | ≥20 |
Cr20ni35 | 1100 ℃ | 1.04 ± 0.05μΩ.m | 1390 ℃ | 750 | ≥20 |
Cr20ni30 | 1100 ℃ | 1.04 ± 0.05μΩ.m | 1390 ℃ | 750 | ≥20 |
Raddied | Cyfansoddiad cemegol% | ||||||||
C | P | S | Mn | Si | Cr | Ni | Al | Fe | |
≤ | |||||||||
0cr21al4 | 0.12 | 0.025 | 0.025 | 0.7 | ≤1.0 | 17-21 | ≤0.6 | 3-4 | mantolwch |
0cr25al5 | 0.06 | 0.025 | 0.02 | 0.5 | ≤0.6 | 23-26 | ≤0.6 | 4.5-6.5 | mantolwch |
0cr23al5 | 0.06 | 0.025 | 0.02 | 0.5 | ≤0.6 | 20.5-23.5 | ≤0.6 | 4.2-5.3 | mantolwch |
0cr21al6nb | 0.05 | 0.025 | 0.02 | 0.5 | ≤0.6 | 21-23 | ≤0.6 | 5-7 | mantolwch |
0cr27al7mo2 | 0.05 | 0.025 | 0.02 | 0.2 | ≤0.4 | 26.5-27.8 | ≤0.6 | 6-7 | mantolwch |
Cr20ni80 | 0.08 | 0.02 | 0.015 | 0.6 | 0.75-1.6 | 20-23 | mantolwch | < 0.5 | ≤1.0 |
Cr15ni60 | 0.08 | 0.02 | 0.015 | 0.6 | 0.75-1.6 | 15-18 | 55-61 | < 0.5 | mantolwch |
Cr20ni35 | 0.08 | 0.02 | 0.015 | 1.0 | 1-3 | 18-21 | 34-37 | - | mantolwch |
Cr20ni30 | 0.08 | 0.02 | 0.015 | 1.0 | 1-3 | 18-21 | 30-34 | - | mantolwch |